PF Power Fittings Technical Reference

AAAC Conductor Table, IEC 61089 Type A2

21 rows · 16 to 1250 mm² · IEC 61089 A2 · 7 to 91 wires

AAAC is All Aluminium Alloy Conductor. The GB/T 1179 designation is JLHA; IEC 61089 writes the alloy as A2, and ASTM B399 calls the same family 6201-T81. No steel, no cladding, no second metal anywhere in the conductor — every wire is the same alloy.

That single fact decides where the type is used. An all-aluminium conductor has no bimetallic joint to corrode, so AAAC goes where a galvanised steel core does not survive: coastal lines, salt fog, industrial pollution. It carries roughly 1.5 to 2 times the tensile strength of AAC at nearly the same weight, which is what buys the longer span.

Nominal Area mm2Number of WiresSingle Wire Dia. mmOverall Dia. mmCalculated Area mm2Weight kg/kmRated Strength kNDC Resistance at 20 °C Ω/km
1671.835.4918.4150.45.431.7896
2572.296.8728.8378.98.491.1453
4072.898.6745.92125.613.580.7158
6373.6310.8972.44198.121.390.4545
100192.7813.90115.33317.033.950.2877
125193.1015.50143.41394.142.440.2302
160193.5117.55183.85505.354.320.1798
200193.9319.65230.48633.467.910.1439
250194.3921.95287.59790.484.880.1151
315373.5324.71362.11999.2106.950.0916
400373.9827.86460.321270.2135.810.0721
450374.2229.54517.511428.0152.790.0641
500374.4531.15575.461587.9169.760.0577
560613.6733.03645.291780.6190.140.0516
630613.8935.01724.972000.5213.900.0458
710614.1337.17817.182254.9241.070.0407
800614.3839.42919.112536.2271.620.0361
900913.8141.911037.482862.8305.580.0321
1000914.0144.111149.263171.3339.530.0289
1120914.2546.751290.953562.2380.270.0258
1250914.4949.391440.873975.9424.410.0231

Nominal Area Is A Label, And It Is Always 15 Per Cent Low

The first and fifth columns are not the same number, and the gap is not a rounding artefact — it is the same on every row:

Nominal Calculated Ratio
16 18.41 1.1506
63 72.44 1.1498
200 230.48 1.1524
500 575.46 1.1509
800 919.11 1.1489
1250 1440.87 1.1527

Fourteen point seven to fifteen point three per cent, over a section range of ninety to one. A ratio that flat is a definition in the standard, not a consequence of which wire was chosen. The practical consequence is one line: weight, rated strength and resistance all follow the calculated area, never the nominal one. Price a tonne against the nominal figure and the order is fifteen per cent short.

The definition is in Annex D, clause D.2.1: Aa = code number × resistivity of Ax ÷ resistivity of A1. A2 alloy is 0.0325 Ω·mm²/m against 0.028264 for A1, a ratio of 1.150, so the alloy conductor needs fifteen per cent more metal to reach the same resistance. That is the whole of the gap, and it is why the same code number sits on two different sections in two tables. The ACSR/AW page uses the same rule and shows it from the other side: resistance times aluminium area is flat across the whole table.

Rated Strength Is Section Times 295 MPa

The strength column is not a tested value with a scatter band. On all twenty-one rows it is the calculated area multiplied by one number:

  • 18.41 mm² × 295 = 5.43 kN, printed 5.43.
  • 460.32 × 295 = 135.79 kN, printed 135.81.
  • 1440.87 × 295 = 425.06 kN, printed 424.41.

Row by row the implied stress runs from 294.4 to 295.9 N/mm² — a spread of half a per cent. So this is a material figure carried straight through, not a stranded-conductor break. A finished conductor loses a few per cent to the helical lay and to uneven tension between layers, exactly as on the GSW page, and the table does not give that derated value. For a tension calculation, derate it.

Weight And Resistance Both Carry A Lay Factor

Weight is the calculated area times the alloy density of 2.69 g/cm³, plus a lay factor that grows with the number of layers:

  • 7-wire rows: 18.41 × 2.69 = 49.5, printed 50.4 — 1.8 per cent over.
  • 19-wire: 115.33 × 2.69 = 310.2, printed 317.0 — 2.2 per cent.
  • 91-wire: 1440.87 × 2.69 = 3875.9, printed 3975.9 — 2.6 per cent.

Resistance runs the same way. At the A2 resistivity of 0.03284 Ω·mm²/m, which is 52.5 per cent IACS, the 16 mm² row calculates to 1.7838 Ω/km against a printed 1.7896, and the 1250 mm² row to 0.0228 against 0.0231. The printed figures are the ones to use; they include the extra length of wire in the lay.

The Diameters Are Exact, Not Rounded

Every overall diameter is a whole multiple of its single-wire diameter:

Wires Construction Diameter
7 1 + 6 3d
19 1 + 6 + 12 5d
37 1 + 6 + 12 + 18 7d
61 1 + 6 + 12 + 18 + 24 9d
91 1 + 6 + 12 + 18 + 24 + 30 11d

All twenty-one rows land on their multiple to the second decimal — 7 × 1.83 = 5.49, 19 × 3.10 = 15.50, 91 × 4.49 = 49.39. There is no allowance for the outer layer standing proud of the nominal circle. A diameter measured across a real drum will read slightly larger than the table.

One Alloy Here, Another In The Standard

IEC 61089 also defines an A3 alloy. Its rated strengths run higher — the same nominal sizes carry more breaking load — and it is not reproduced on this page. Mixing two grades in one list without a grade column is how a reader ends up specifying a strength the supplier cannot meet.

The ASTM counterpart is B399, which lists the same family under code words — Akron, Alton, Ames — sized in kcmil instead of mm², and stranded to its own sizes. The two lists do not map one row to one row: an IEC 16 mm² row is seven wires of 1.83 mm calculating to 18.41 mm², and the nearest B399 size is not the conductor of the same nominal figure. A tender written against an ASTM code word cannot be filled from this table alone.

What Is Missing

  • No ampacity. The standard gives none; it depends on wind, ambient and allowable temperature.
  • No modulus, no coefficient of expansion, no sag. Needed for a stringing calculation, absent from the table.
  • No A3 rows.
  • No kcmil code words, so no direct lookup against an ASTM tender.

The other conductor tables: ACSR, AAC, AACSR/AW, GSW, TACSR, expanded diameter. Back to the designation reference.

Note: Twenty-one rows, IEC 61089 A2. The calculated area sits 14.7 to 15.3 per cent above the nominal figure on every row, so nominal area is a label; weight, strength and resistance all follow the calculated figure. Rated strength is calculated area times 295 N/mm² within half a per cent, which makes it a material figure rather than a stranded-conductor break. Weight and resistance carry a lay factor rising from 1.8 per cent at seven wires to 2.6 per cent at ninety-one.